Purpose: performance evaluation of XOANONS
®WE-D210
1.Dispersing titanium white in polyester amino resin system
1.1 grinding prepare
| Component |
Dosage(g) |
| Saturatedpolyesterresin |
30 |
| Dispersingagent |
0.7 |
| Titaniumwhite(BLR-699) |
35 |
| Mixedsolvent |
11.1 |
| Total |
76.8 |
1.2 fineness and viscosity
| Storagetime |
Dispersingagent |
fineness |
viscosity |
| 1h |
2h |
|
| Beforestorage |
Similarproduct |
15 |
15 |
Thesamewithalowviscosity |
| XOANONS®WE-D210 |
15 |
15 |
| Storefor10dayat50℃ |
Minimalchanginginfinenessandviscosity |
1.3 Preparation of paint. Distribute the paint over the black&white cardboard. Drying for 1min at 280℃.
| Component |
Dosage(g) |
| Whitepaste |
76.8 |
| Saturatedpolyesterresin |
12 |
| Methylatedaminoresin |
8 |
| XOANONS®WE-D887 |
0.4 |
| Acidcatalyst |
0.4 |
| Mixedsolvent |
2.4 |
| Total |
100 |
1.4 data sheet before storage
| Dispersingagent |
opacity |
L |
20°gloss |
| Similarproduct |
86.83 |
94.02 |
62.60 |
| XOANONS®WE-D210 |
87.40 |
94.10 |
63.40 |
1.5 data sheet after storage 10days at 50℃
| Dispersingagent |
opacity |
L |
20°gloss |
| Similarproduct |
86.04 |
93.74 |
64.60 |
| XOANONS®WE-D210 |
87.95 |
93.91 |
65.40 |
2. Dispersing titanium white in thermoplastic acrylic resin system 2.1 grinding prepare
| Component |
Dosage(g) |
| Thermoplasticacrylicresin |
59.7 |
| Dispersingagent |
0.3 |
| Titaniumwhite(BLR-699) |
30 |
| Mixedsolvent |
10 |
| Total |
100 |
2.2 fineness and viscosity
| Storagetime |
Dispersingagent |
fineness |
viscosity |
| 1h |
2h |
|
| Beforestorage |
Similarproduct |
15 |
15 |
Thesamewithalowviscosity |
| XOANONS®WE-D210 |
15 |
15 |
| Storefor10dayat50℃ |
Minimalchanginginfinenessandviscosity |
2.3 Preparation of paint
2.3.1 medium-gloss paint: Dilute paste(5g) with solvent(2g). Distribute the paint over the black&white cardboard.Self-drying.
2.3.2 high-gloss paint: Dilute paste(3g) with solvent(2g) and resin(3g). Distribute the paint over the black&white cardboard.Self-drying.
2.4 data sheet before storage
| Item |
Dispersingagent |
opacity |
L |
20°gloss |
60°gloss |
| Medium-gloss |
Similarproduct |
73.50 |
94.25 |
—— |
59.90 |
| XOANONS®WE-D210 |
74.45 |
94.38 |
—— |
61.70 |
| High-gloss |
Similarproduct |
69.03 |
93.74 |
61.00 |
—— |
| XOANONS®WE-D210 |
69.89 |
93.79 |
63.30 |
—— |
2.5 data sheet after storage 10days at 50℃
| Item |
Dispersingagent |
opacity |
L |
20°gloss |
60°gloss |
| Medium-gloss |
Similarproduct |
73.29 |
94.14 |
—— |
65.30 |
| XOANONS®WE-D210 |
74.32 |
94.26 |
—— |
65.20 |
| High-gloss |
Similarproduct |
77.85 |
93.67 |
65.70 |
—— |
| XOANONS®WE-D210 |
78.04 |
93.82 |
66.80 |
—— |
3. Dispersing titanium white in hydroxyl acrylic resin system 3.1 Grinding prepare
| Component |
Dosage(g) |
| Hydroxylacrylic |
33.6 |
| Dispersingagent |
0.5 |
| Titaniumwhite(BLR-699) |
50 |
| Mixedsolvent |
15.9 |
| total |
100 |
3.2 fineness and viscosity
| Storagetime |
Dispersingagent |
fineness |
viscosity |
| 1h |
2h |
|
| Beforestorage |
Similarproduct |
15 |
12.5 |
Thesamewithalowviscosity |
| XOANONS®WE-D210 |
15 |
12.5 |
| Storefor10dayat50℃ |
Minimalchanginginfinenessandviscosity |
3.3 Preparation of paint. Paste(4g) + hydroxyl acrylic resin(1g)+ solvent(2g)+ curing agent(1g). Distribute the paint over the black&white cardboard. Drying for 30min at 90℃. 3.4 data sheet before storage
| Dispersingagent |
opacity |
L |
20°gloss |
| Similarproduct |
73.91 |
93.95 |
80.30 |
| XOANONS®WE-D210 |
74.06 |
93.94 |
81.90 |
3.5 data sheet after storage 10days at 50℃
| Dispersingagent |
opacity |
L |
20°gloss |
| Similarproduct |
76.30 |
94.28 |
81.60 |
| XOANONS®WE-D210 |
77.90 |
94.38 |
81.20 |
4. Dispersing titanium white in alkyd resin 4.1 grinding prepare
| Material |
Dosage(g) |
| Alkydresin(dilutedtocontent50%) |
33.6 |
| Dispersingagent |
0.5 |
| Titaniumwhite(BLR-699) |
50 |
| Mixedsolvent |
15.9 |
| total |
100 |
4.2 fineness and viscosity
| Storagetime |
Dispersingagent |
fineness |
viscosity |
| 1h |
2h |
|
| Beforestorage |
Similarproduct |
15 |
12.5 |
Thesamewithalowviscosity |
| XOANONS®WE-D210 |
15 |
12.5 |
| Storefor10dayat50℃ |
Minimalchanginginfinenessandviscosity |
4.3 preparation of paint Paste(4g)+ alkyd resin(1g)+ solvent(2g)+ curing agent(1g). Distribute the paint over the black&white cardboard. Drying in 30min at 90℃. 4.4 data sheet before storage
| Dispersingagent |
opacity |
L |
20°gloss |
| Similarproduct |
74.22 |
93.62 |
83.00 |
| XOANONS®WE-D210 |
75.13 |
93.68 |
82.80 |
4.5 data sheet after storage 10days at 50℃
| Dispersingagent |
opacity |
L |
20°gloss |
| Similarproduct |
76.28 |
94.02 |
83.40 |
| XOANONS®WE-D210 |
76.78 |
93.28 |
83.60 |
Note:Opacity indicates the ability of the substrate surface coating cover color. Higher value, better covering power. L means light. Higher value, much whiter of coat film and vice versa.